PVC-1 40 Mil Lining Physical Properties Chart |
| Thickness | ASTM D-751 | .040 Inches (1 mm) Nominal |
| Installed Weight (w/o any Ballast) | ASTM D-751 | .25 LBS. Per Sq.Ft. (1.2 KG Per M2) |
| Tearing Strength Tongue Method | ASTM D-5587 Trapezoidal Tear | 130 X 110 Lbs. (578 X 489N) |
| Breaking Strength | ASTM D-751 | 435 X 350 Lbs. (1933 X 1557N) |
| Tensile Strength | ASTM D-751 & ASTM D-882 | 7200 PSI |
| Emmaqua Exposure | ASTM G-90 Desert Sun | 8.1 Million Langleys (339,790260 MJ/M2) |
| Elongation at Break | ASTM D-751 | 35 % |
| Dimensional Stability | ASTM D-1204 | <0.1% |
| Low Temperature Flexibility | ASTM D-2136 1/8" (3.2 MM) Mandrel | -40° F (-40° C) No Cracks |
| Heat Aging | ASTM D-3045 7 Days @ 194° F | Retains 90 % of Breaking Strength >95% of Elongation |
| Permeability | ASTM E-96, PRO BW ASTM E-96,WVT,Proc,B,M,A | .25 U.S. Perms (.086 G/Hr./MXM) |
| Shore of Hardness | ASTM D-2240 | 77 |
| Fungi Resistance | ASTM G-21 | No Sustained Growth or Discoloration |
| Dynamic Impact (Puncturing) | ASTM D 5635 | 474 PDL-Ft. (20J) |
| Water Vapor Transmission | ASTM E-96 WVT Procedure B, Method A | <0.25 U.S. Perms (0.086 G/H/M2) |
| Accelerated Weathering | Carbon Arc 6000 Hrs. | No Cracks, Crazing or Blistering |
| Accelerated Weathering UVB-313 LAMP @ 80° C (176° F) | ASTM G-5388 6000 Hrs. | No Cracks, Crazing or Blistering |
| Factory Mutual Research | ASTM E-108 | Class 1-60,1-90,1-150,1-210 |
| Underwriters Laboratories | UL-790, UL-1897 | Class A,B, or C / UL-150 |